S700MC is a high-strength steel suited to cold forming, widely used in trailer chassis, crane booms, tippers and construction machinery to save weight. Welded correctly, it carries the same load as S355 with much thinner sections. Welded incorrectly, the weld zone can end up considerably weaker than the steel itself.

What Is S700MC?

In S700MC to EN 10149-2, M means thermomechanically rolled and C suitable for cold forming. Minimum yield strength is 700 MPa and tensile strength 750–950 MPa. Its strength comes not from high carbon but from controlled rolling and micro-alloying. The carbon equivalent is therefore low and weldability good, but the steel is sensitive to heat.

The Real Risk: HAZ Softening

In thermomechanical steels, if the heat-affected zone (HAZ) overheats and cools slowly, the fine grain structure gained in rolling is lost and the zone softens. The result is a strip of reduced strength beside the weld. This softening must be controlled at least as much as cracking.

t8/5 Cooling Time and Heat Input

The control measure is t8/5, the cooling time of the weld zone from 800 °C to 500 °C. A short t8/5 gives a hard, crack-prone structure; a long t8/5 gives softening and loss of toughness. For S700MC manufacturers usually recommend roughly 5–15 seconds; take the exact value from the steel maker’s welding guide.

t8/5 depends on heat input, plate thickness, joint type and preheat. Heat input is calculated as:

Q (kJ/mm) = k × U × I × 60 / (v × 1000), where U is voltage (V), I current (A), v travel speed (mm/min) and k the thermal efficiency (0.8 for MAG).

Example: MAG at 26 V, 240 A and 400 mm/min gives Q = 0.8 × 26 × 240 × 60 / 400,000 ≈ 0.75 kJ/mm. Thin plate needs lower and thick plate slightly higher heat input for the same t8/5 range.

Practical Rules

  • Narrow multi-pass welding instead of wide weaving: one large pass raises heat input.
  • Limit interpass temperature: per the manufacturer, usually an upper limit of about 100–150 °C.
  • Preheat: usually not needed on thin plate thanks to the low carbon equivalent; apply for thick sections, high restraint, low ambient temperature or moisture (see preheat calculation).
  • Hydrogen control: clean, dry surfaces and low-hydrogen consumables.
  • Balanced sequence on long welds: split the weld and work alternately so heat does not build up in one area.

Filler: Matching or Undermatching?

For load-bearing butt welds, a matching-strength wire is usually chosen, such as class 69 MAG wires to ISO 16834. For low-stressed fillet welds, an undermatching wire may be preferred; it increases weld metal ductility and lowers crack risk. Which to use should be decided in the design calculation.

What Not to Do

  • Normalizing and hot forming: destroy the thermomechanical structure; the strength does not come back.
  • Stress-relief annealing: generally not recommended; if needed, get the steel maker’s approval.
  • Excess temperature in flame straightening: local heating must not exceed the steel’s permitted temperature.

Qualification

S700MC should be welded with a WPS based on a WPQR qualified to ISO 15614-1. Hardness and tensile tests in the procedure qualification show that HAZ softening stays within acceptance limits (see S960QL welding parameters).

At ArmaWeld: on high-strength steel parts we keep heat input within the range defined in the WPS and measure and record interpass temperature. For long-seam chassis and boom work we use a balanced welding sequence and controlled parameters. Our welded fabrication service →

Frequently Asked Questions

Does S700MC need preheating?

Usually not on thin plate because of the low carbon equivalent. For thick sections, high restraint, cold conditions or moisture, preheat per the manufacturer.

What t8/5 is right for S700MC?

Manufacturers usually recommend roughly 5–15 seconds. Take the exact value from the steel maker’s welding guide.

Which wire is used for S700MC?

Matching-strength wire (e.g. ISO 16834 class 69) for load-bearing butt welds; undermatching wire may be used for low-stressed fillet welds.

Can S700MC be normalized?

No. Normalizing and hot forming destroy the thermomechanical structure and permanently reduce strength.

Controlled welding of high-strength steel

Send your S700MC chassis, boom or platform drawing; we will reply with a welding plan and quotation.

Request a Quote →