Visual testing (VT) looks like the simplest method in weld quality control, yet it catches the most defects. Surface-breaking cracks, undercut, incompletely filled grooves, insufficient throat thickness and geometric deviations are mostly found visually. Properly performed VT also makes later UT or RT meaningful. The standard for the method is EN ISO 17637.

What Does ISO 17637 Define?

The standard defines how visual testing of fusion welds is performed: testing conditions, tools, timing and reporting. It does not give acceptance criteria; acceptance normally follows EN ISO 5817 (steel) or EN ISO 10042 (aluminium).

Testing Conditions

  • Lighting: at least 350 lx on the surface, preferably 500 lx.
  • Viewing distance and angle: eye no more than 600 mm from the surface, viewing angle not less than 30° to the surface.
  • Access: mirrors, borescopes or cameras where direct viewing is not possible.
  • Surface: free of slag, spatter and dirt, otherwise defects are hidden.

When Is It Done?

VT is not only a check after welding. Good practice applies it in three stages:

StageWhat is checked
Before weldingGroove angle, root gap, root face, cleanliness, tack welds, fit-up and misalignment
During weldingInter-pass cleaning, root pass condition, interpass temperature, surface after back-gouging
After weldingWeld dimensions, surface defects, spatter and arc strikes, distortion, cleanliness

A groove error caught before welding is far cheaper to fix than the lack of fusion found afterwards.

Features Measured After Welding

  • Fillet welds: throat thickness a and leg length z, concavity or convexity, unequal legs.
  • Butt welds: cap height, excess root penetration, incompletely filled groove, misalignment, root concavity.
  • Both: undercut depth, surface porosity, crater cracks, weld starts and stops, spatter, arc strikes.

Tools Used

  • Multi-purpose weld gauge (throat, cap height, undercut depth, groove angle)
  • Fillet weld gauge set
  • Calliper, rule and tape measure
  • Magnifier (2x–5x), torch, mirror
  • Surface thermometer where needed (interpass temperature)

What Should a VT Report Contain?

Part and weld identification, applied standard and acceptance level, testing stage, tools used, measured values, location and size of indications, result and inspector details. Recording measured values for accepted welds as well shows the report is a real measurement record.

Competence of VT Personnel

EN 1090-2 and ISO 3834 require VT personnel to be competent. In practice this means VT certification to ISO 9712 or training as welding coordination personnel. Inspectors' eyesight (near vision acuity, colour perception) should also be checked regularly.

Limits of VT

Visual testing only sees the surface. Internal porosity, internal cracks and lack of fusion cannot be found with VT; UT or RT is needed. Very fine surface cracks may also be missed; suspicious areas get PT or MT. VT should therefore be seen as the first link of the NDT plan, not as a stand-alone check.

At ArmaWeld: every weld is visually tested to ISO 17637 by our ISO 9712 Level 2 VT certified personnel, and measured values are entered in the report. On critical parts, pre-weld groove checks are also recorded. See our quality approach →

Frequently Asked Questions

What is the minimum lighting for VT?

ISO 17637 requires at least 350 lx on the surface and recommends 500 lx. Where workshop lighting is insufficient, a torch or portable lamp is used.

Is certification required for visual testing?

EN 1090-2 and ISO 3834 require competent personnel. Customer specifications usually ask for VT Level 2 certification to ISO 9712.

When should VT be performed?

Before welding (groove and fit-up), during welding (between passes) and after welding. For high-strength steels at risk of delayed cracking, final inspection follows the hold time given in the standard.

Which standard gives VT acceptance criteria?

ISO 17637 does not. Steel usually uses the quality levels of EN ISO 5817, aluminium those of EN ISO 10042.

Welded parts with every weld measured and reported

Send your drawing and we will state the VT and NDT scope clearly in our quotation.